How to calculate UV curing dose in mJ/cm² (without guessing)

Most cure failures are dose failures, not lamp failures. Here is the arithmetic that turns a datasheet number into a belt speed and a working distance.

If an adhesive datasheet says 2 J/cm², that is a target for energy delivered to the bond line — not a time, and not a lamp setting. Getting from one to the other takes two measured numbers and one multiplication. Engineers who skip this step end up turning the power up until the part feels dry, which is how over-cure, warping and brittle joints happen.

Dose is energy per area, so time is a variable

Irradiance (mW/cm²) is how hard the light hits. Dose (mJ/cm²) is how much energy landed over the exposure. Multiply one by the other:

Dose (mJ/cm²) = Irradiance (mW/cm²) × Time (s)

A point source measured at 1,200 mW/cm² curing for 2 s delivers 2,400 mJ/cm², or 2.4 J/cm². If the datasheet asks for 2 J/cm², 2 s is enough with margin; 1 s would leave you at 1,200 mJ/cm², roughly 40% short. That gap is exactly the difference between a joint that passes a pull test on Monday and one that fails in the field.

Watch the units on the datasheet. Suppliers mix J/cm², mJ/cm² and occasionally mJ/mm². One J/cm² is 1,000 mJ/cm².

Typical dose bands, as a starting point

These are common ranges for common jobs. They are for orientation only — the adhesive supplier's number always wins, because photoinitiator loading and pigment content change the requirement by an order of magnitude.

Typical dose targets by process (starting points, verify with the adhesive datasheet)
ProcessTypical doseNotes
Inkjet pinning20–100 mJ/cm²Enough to freeze the drop, not to cure it
Structural UV acrylate bond500–3,000 mJ/cm²Clear adhesive, bond line under 1 mm
Screen ink, 10–30 µm wet1,000–5,000 mJ/cm²Thick layer, surface cure leads through-cure
Pigmented or filled adhesive3,000–8,000 mJ/cm²Titanium dioxide and carbon black absorb UV
Conformal coating1,000–4,000 mJ/cm²Shadowed component sides need a second pass

Measure at the part, not at the lamp

The irradiance printed on a test report is measured at a stated distance — usually 10 mm for a point head, at the window for an area source. Mount the radiometer at the bond line and the reading will be lower: distance costs you energy, and fixtures rarely let you work at the rated gap.

Distance matters more than people expect, because intensity falls roughly with the square of the distance. Doubling the working distance from 10 mm to 20 mm leaves about a quarter of the irradiance, so the same 2 s exposure delivers a quarter of the dose.

100%1025%2011%306%40working distance, mm
Relative irradiance against working distance for a point source. Inverse-square estimate — measure your own fixture, the real curve is flatter close in and depends on the lens.

Conveyor lines: dose comes from belt speed

On a moving web or belt you do not set a timer, so the exposure time is the time the part spends under the emitting window:

Time (s) = window length (mm) ÷ belt speed (mm/s)
Dose (mJ/cm²) = Irradiance (mW/cm²) × Time (s)

A 250 mm line source over a belt running at 5 m/min: 5 m/min is 83 mm/s, so each point is under the window for 250 ÷ 83 = 3.0 s. At a measured 1,000 mW/cm² that is 3,000 mJ/cm². Halve the belt speed and you double the dose — which is why belt speed is the first thing to check when a coating stops curing after a line speed increase.

Four things that quietly cut your dose

  • Distance drift. A fixture that moved 5 mm during maintenance can halve the irradiance. Mark the working gap on the fixture and re-check it after every changeover.
  • Thermal derating. LED output drops as the die heats. A water-cooled array held at 25 °C holds its number; an air-cooled head in a closed cabinet may be 10–20% down after an hour. Measure hot, not cold.
  • A dirty window or lens. A fingerprint on a quartz window is a diffuser, not a transparent surface. Wipe with isopropyl alcohol and re-measure.
  • Radiometer mismatch. A 365 nm-calibrated sensor reads low at 395 nm and vice versa. Use a sensor calibrated for your peak wavelength, and re-certify it annually.

A worked example

A medical assembly cell bonds a 3 mm catheter joint with a clear acrylate rated at 1.5 J/cm². A Ø10 mm point head reads 1,600 mW/cm² at the fixture gap. Required time: 1,500 ÷ 1,600 = 0.94 s. Round to 1.5 s for margin and for the operator’s foot-pedal reaction: that delivers 2,400 mJ/cm², a 60% cushion. The cushion is not waste — it absorbs LED ageing over the 20,000 h life and the day someone forgets to clean the window.

The short version

  • Dose = irradiance × time. Time = window length ÷ belt speed.
  • Measure irradiance at the bond line with the machine at working temperature.
  • Design in 30–60% margin so ageing and dirt do not put you under the datasheet number.
  • Re-check irradiance every three to six months with a calibrated radiometer.

Questions on this topic

Is more dose always safer?

No. Over-cure makes acrylates brittle, can yellow clear parts, and warps thin substrates through shrinkage stress. Aim for the datasheet band with a sensible margin rather than running the lamp at 100% because it feels safer.

Can I compute dose from the lamp’s electrical power?

Not usefully. Electrical power says nothing about optical output at the part plane, because lensing, distance and cooling all sit in between. A $200 radiometer replaces the guesswork and is the cheapest process instrument you will buy.

How often should the radiometer be recalibrated?

Annually for production use, and any time it is dropped or left in a hot cabinet. An out-of-calibration sensor reads high, which means you under-dose without noticing until parts fail.